title: Contact Materials and Plating Compared | ACA Atlas Contacte
description: "Contact materials compared: CuSn, CuBe, CuNiSi, CuFeP, brass, copper and spring steels. Plus silver, tin, gold or nickel plating and when to use which."
url: https://www.atlas-contacte.de/en/knowledge/materials-finishes/
lang: en-GB
alternate:
  de: https://www.atlas-contacte.de/de/wissen/werkstoffe-oberflaechen/
alternate_markdown:
  de: https://www.atlas-contacte.de/de/wissen/werkstoffe-oberflaechen/index.md
last_updated: 2026-11-14
breadcrumb: Home > Knowledge > Materials and finishes
publisher: ACA Atlas Contacte GmbH
---

# Contact materials and finishes

Which material for contact springs, contact lamellae and stamped parts, and which finish on top? This guide from ACA Atlas Contacte GmbH in Wehr (Baden), Germany, compares the copper alloys and spring steels that ACA processes, and the common contact platings, by conductivity, spring properties and application.

## Conductivity or spring force: the basic trade-off

A contact material has to do two jobs at once: carry current and provide contact force. The two requirements pull in opposite directions. Pure copper conducts extremely well but hardly acts as a spring. Alloying elements such as tin, beryllium, nickel with silicon, or iron make copper stronger and springier, but lower its electrical conductivity. Every choice of material is therefore a trade-off between current, force, temperature, formability and price.

Conductivity is often stated in percent IACS (International Annealed Copper Standard). 100 % IACS corresponds to 58 MS/m at 20 °C, the conductivity of annealed pure copper. Electrolytic tough pitch copper, Cu-ETP, typically reaches around 100 % IACS and is therefore the benchmark for every other contact material.

The second property is often underestimated in practice: resistance to stress relaxation. A spring that works under preload at elevated temperature loses part of its force over time. As the contact force drops, contact resistance rises, the contact runs hotter and relaxation accelerates. For contacts that stay warm in service, stress relaxation resistance often matters more than conductivity in the as-new condition.

**Fig. 1: Conductivity versus spring properties.** Qualitative ranking from the table “Contact materials compared”, not property values. Alloying elements make copper stronger and springier but lower its conductivity.

## Contact materials compared

| Criterion | Conductivity | Spring properties | Stress relaxation resistance | Bendability | Cost level |
| --- | --- | --- | --- | --- | --- |
| Copper (Cu-ETP) | very high, typically around 100 % IACS | low | low | very good | medium |
| Copper-iron-phosphorus (CuFeP) | high | medium | medium | good | low to medium |
| Copper-nickel-silicon (CuNiSi) | medium to high | high | very good | medium to good | medium to high |
| Beryllium copper (CuBe) | medium | very high | very good | good before age hardening | high |
| Phosphor bronze (CuSn) | low | high | medium | good | medium |
| Brass (CuZn) | medium | low to medium | low | very good | low |
| Stainless spring steel | very low | very high | very good | medium | medium |
| Carbon spring steel | very low | very high | good | limited when hardened | low |

ACA Atlas Contacte processes all eight materials in this table, stainless spring steel for example as 1.4310 and carbon spring steel as C75S. The ranking is qualitative and for orientation only, not property values. Actual values depend on alloy, temper and mill. The material standard and the strip supplier's datasheet are binding.

## Copper and copper alloys for contacts

ACA processes these materials into [stamped and bent parts to drawing](https://www.atlas-contacte.de/en/products/stamped-bent-parts/).

- **Copper (Cu-ETP)** (CW004A): Cu-ETP is the default material when carrying current is the main task and little spring force is needed: contact pieces, connection parts and current paths. Copper bends very well but quickly loses force under heat and preload. Where spring force is needed, a second material provides it. In the ACA [high-current contact band](https://www.atlas-contacte.de/en/products/louvered-contact-bands/high-current-contact-band/), contact pieces of high-conductivity copper are riveted onto a carrier strip of stainless spring steel.
- **Copper-iron-phosphorus (CuFeP)** (e.g. CuFe2P, CW107C): CuFeP sits between copper and the classic spring bronzes: considerably stronger than copper while keeping high conductivity. Typical uses are connectors, terminal tabs and parts with a moderate spring function that carry a lot of current and do not run hot continuously. It forms well and plates well.
- **Copper-nickel-silicon (CuNiSi)** (e.g. CuNi2Si, CW111C): CuNiSi alloys are precipitation-hardening. They combine high strength with good conductivity and very good stress relaxation resistance. That makes them suitable for contact springs and plug contacts that stay warm in service, for example in power electronics or charging connectors. CuNiSi is also the obvious beryllium-free alternative when beryllium copper is not wanted.
- **Beryllium copper (CuBe)** (e.g. CuBe2, CW101C): After [age hardening](https://www.atlas-contacte.de/en/knowledge/glossary/#term-age-hardening), beryllium copper reaches the highest strength of all copper alloys and keeps its spring force at elevated temperature. That is why ACA makes its [leaf spring contact band](https://www.atlas-contacte.de/en/products/louvered-contact-bands/leaf-spring-contact-band/) and its [torsion spring contact band](https://www.atlas-contacte.de/en/products/louvered-contact-bands/torsion-spring-contact-band/) from CuBe only. CuBe is either formed in the solution-annealed condition and age-hardened afterwards, or processed as mill-hardened strip that needs no further heat treatment. ACA processes both conditions, depending on the part, and age-hardens solution-annealed CuBe in-house after forming. Operations that create dust or fumes, such as grinding or welding, require protective measures. REACH information duties apply to beryllium-containing articles along the supply chain. ACA provides REACH Article 33 information on beryllium as a substance of very high concern (SVHC) for CuBe parts on request.
- **Phosphor bronze (CuSn)** (e.g. CuSn6, CW452K): Tin bronze, usually called phosphor bronze, is the classic spring material of electrical engineering: strong, easy to bend, easy to solder and plate, and available in many tempers. Its weak points are comparatively low conductivity and moderate stress relaxation resistance at higher temperatures. For [contact springs](https://www.atlas-contacte.de/en/products/contact-springs/), clamping springs and signal contacts at normal ambient temperature, CuSn is often the most economical choice.
- **Brass (CuZn)** (e.g. CuZn37, CW508L): Brass is inexpensive, forms very well and conducts better than phosphor bronze. It is of limited use for springs because it relaxes quickly under load. Typical applications are [flat tabs](https://www.atlas-contacte.de/en/products/plug-contacts/flat-tabs-receptacles/), solder tags, terminal clamp bodies and connection parts without a permanent spring function.

## Stainless and carbon spring steel

- **Stainless spring steel** (e.g. 1.4310 (X10CrNi18-8)): Stainless spring steel offers high spring force, very good stress relaxation resistance and corrosion resistance, but conducts poorly. It suits retaining springs, spring clips and clamping springs, and any design where the spring provides the force while another material carries the current. In the ACA high-current contact band, stainless spring steel forms the carrier strip that generates the contact force.
- **Carbon spring steel** (e.g. C75S (1.1248)): Carbon spring steel is the most economical route to high spring force, for example for retaining and locking springs without an electrical function. It needs corrosion protection. When high-strength steels are electroplated, the process sequence must take the risk of hydrogen embrittlement into account.

## Choosing a material: four rules of thumb

The starting point is not the material but the function of the part. The following rules lead to the right material family in most cases. We then select the alloy and temper together with you, matched to deflection, force and temperature.

- **High current, little deflection:** copper or CuFeP, silver or tin plated.
- **Spring force at elevated temperature:** CuBe or CuNiSi, for their stress relaxation resistance.
- **Spring force at room temperature on a tight budget:** CuSn, or brass if the spring function is minor.
- **Separate force and current:** a steel spring for the force, copper for the current, joined by riveting or welding.

## Silver, tin, gold or nickel: finishes compared

| Criterion | Contact resistance | Required contact force | Mating cycles | Cost level | Typical use |
| --- | --- | --- | --- | --- | --- |
| Silver (Ag) | very low | medium | medium to high, with passivation or lubrication | medium | high current, power contacts, contact lamellae |
| Tin (Sn) | low, as long as the oxide film is broken | high | low | low | solder terminations, rarely mated connections |
| Gold (Au) | very low and stable | low | high | high | signal and measuring contacts, low currents and voltages |
| Nickel (Ni) | medium to high, due to oxide film | high | medium | low to medium | barrier layer under Au, Ag or Sn, wear and corrosion protection |

Tendencies for common thicknesses and layer systems. How a finish behaves in service depends on thickness, underlayer, contact force, mating contact and environment.

## Which finish when?

- **Silver (Ag)** (silver plated, passivated): Silver has the highest electrical conductivity of all metals and forms no insulating oxide. That makes it the usual finish for high-current contacts and high-current contact lamellae. In sulphur-bearing atmospheres silver tarnishes. At low contact force the sulphide film can raise contact resistance, and a passivation delays tarnishing. When sliding, silver tends to cold-weld, so a low-friction passivation or a contact lubricant reduces friction and wear. The ACA torsion spring contact band is silver plated and passivated as standard, and the contact pieces of the high-current contact band carry 20 µm of silver as standard.
- **Tin (Sn)** (electroplated or hot-dip tinned): Tin is the economical finish for solder terminations and for connections that are rarely mated. Tin is soft and oxidises in air. The oxide film has to be broken by sufficient contact force on mating. Under vibration and temperature cycling, tin-plated contacts are prone to fretting corrosion, because every micro-movement creates fresh oxide. With pure electroplated tin, whiskers can also grow, especially at tight spacings in electronics.
- **Gold (Au)** (gold plated, usually hard gold over nickel): Gold does not oxidise and keeps contact resistance stable even at low contact force, low current and low voltage. That makes gold the first choice for signal, measuring and data contacts and for contacts with many mating cycles. Plug contacts usually use thin, hardened gold layers over a nickel barrier. Because gold is expensive, it is often applied selectively to the contact zone only.
- **Nickel (Ni)** (nickel plated, also as underlayer): Nickel is hard, wear-resistant and corrosion-resistant. As an underlayer it stops copper and zinc diffusing from the base material into the top layer and so extends the life of gold, silver and tin finishes. As a contact surface, nickel forms a thin oxide film and needs higher contact forces. For contact lamellae in standard applications, nickel is an economical option: the ACA [leaf spring contact band](https://www.atlas-contacte.de/en/products/louvered-contact-bands/leaf-spring-contact-band/) is available nickel, silver or gold plated.
- **Selective plating** (partial or stripe plating): With selective plating, only the functional zone receives the expensive layer, for example gold on the contact zone and tin on the solder termination. This saves precious metal and is common for reel-to-reel plated parts. ACA supplies [electroplated and selectively plated strip](https://www.atlas-contacte.de/en/products/contact-strips/) and processes clad strip and contact profiles. Plating is carried out by specialised partner companies, see [surface finishes](https://www.atlas-contacte.de/en/services/surface-finishes/).

## Layer systems and the right sequence

A finish is rarely a single layer. A typical build-up is base material, nickel barrier and a top layer of gold, silver or tin. For the design, it also matters when plating takes place: before stamping, afterwards on the strip, or as loose parts. The sequence determines edge protection, formability and cost.

- **Pre-plated strip:** economical in large quantities. Cut edges stay unplated, and bends are formed through the finished layer.
- **Plating after stamping, on the strip:** edges are plated too, selective zones are possible, and the parts stay on the carrier strip for further processing.
- **Barrel plating of loose parts:** for parts that are to be plated all over. Not suitable for delicate geometries that tangle.

**Fig. 2: Layer system and plating sequence.** A finish is rarely a single layer. The order of stamping and plating decides edge protection, formability and cost.

- A Layer build-up: Base material, nickel barrier layer and a top layer of gold, silver or tin.
- B Pre-plated strip: Economical in high volumes. The cut edges stay unplated.
- C Plated after stamping: The edges are plated too, and selective zones are possible.
- D Selective plating: For example gold on the contact zone and tin on the solder tail.

## The mating contact counts too

A contact is always a pair. The basic rule: identical or compatible finishes on both sides. Gold against tin is considered a poor pairing, because the soft tin transfers onto the gold during micro-movements and oxidises there.

The base material of the mating contact also affects the current rating. According to the datasheets for our contact bands, the resistance per web rises by around 40 % when the mating contact is silver-plated brass instead of silver-plated copper. The permissible current then falls to 60 % of the value for copper. If you make the pin and socket yourself, choose their material and finish as carefully as the lamella.

## Example: materials and finishes of ACA contact lamellae

| Property | Value |
| --- | --- |
| Leaf spring contact band · base material | beryllium copper (CuBe), relaxation-resistant |
| Leaf spring contact band · finish | nickel, silver or gold |
| Torsion spring contact band · base material | beryllium copper (CuBe), relaxation-resistant |
| Torsion spring contact band · finish | silver plated and passivated, alternatively bare |
| Torsion spring contact band · silver layer | on request |
| High-current contact band · carrier strip | stainless spring steel |
| High-current contact band · contact pieces | copper, silver plated, passivated for low friction |
| High-current contact band · copper contact thickness | 0.6 mm |
| High-current contact band · silver layer (standard) | 20 µm |

Data from ACA datasheets, installation drawings and the previous product page. Layer thicknesses on request. The leaf spring and torsion spring contact bands are made only from CuBe. Details per design on the [contact lamellae](https://www.atlas-contacte.de/en/products/louvered-contact-bands/) page.

## Frequently asked questions

### Which material is best for contact springs?

It depends on current, temperature and deflection. For contact springs at room temperature, phosphor bronze (CuSn) is often the most economical choice. If the springs stay warm in service, beryllium copper (CuBe) or CuNiSi are better because of their stress relaxation resistance. If a lot of current has to flow, CuFeP or a combination of a steel spring and a copper conductor are worth considering.

### Silver or tin: which finish is better for plug contacts?

Silver suits high currents, higher temperatures and more frequent mating. Tin is the low-cost choice for solder terminations and rarely mated connections with sufficient contact force. Tin-plated contacts are prone to fretting corrosion under vibration. Silver-plated contacts should be passivated or lubricated so that they do not cold-weld when sliding.

### When is gold plating of contacts worth it?

Gold plating pays off at low currents and voltages, for measuring and signal contacts and for many mating cycles. Gold forms no oxide and keeps contact resistance stable even at low contact force. To save cost, gold is usually applied thinly over a nickel barrier and often only selectively on the contact zone.

### What does % IACS mean for contact materials?

% IACS states electrical conductivity relative to annealed pure copper according to the International Annealed Copper Standard. 100 % IACS corresponds to 58 MS/m at 20 °C. Electrolytic copper Cu-ETP is typically around 100 % IACS, spring alloys such as phosphor bronze or beryllium copper are well below that.

### Is there an alternative to beryllium copper for contact springs?

Yes. CuNiSi alloys reach high strength and very good stress relaxation resistance without beryllium and conduct current well. Whether they are sufficient for a specific spring depends on deflection, force and temperature. ACA Atlas Contacte GmbH also makes contact springs to drawing from CuNiSi. The ACA leaf spring and torsion spring contact bands, by contrast, are always made from CuBe.

## Related pages

- [Contact types compared](https://www.atlas-contacte.de/en/knowledge/contact-types-compared/): Which contact type suits your current, mating cycles and space
- [Designing stamped parts](https://www.atlas-contacte.de/en/knowledge/designing-stamped-parts/): Rules of thumb for bend radii, hole diameters, web widths and tolerances
- [Surface finishes](https://www.atlas-contacte.de/en/services/surface-finishes/): Electroplated finishes through qualified partners
- [Glossary](https://www.atlas-contacte.de/en/knowledge/glossary/): Stamping and contact technology terms, explained briefly and precisely

## Define material and finish together

Tell us the current, temperature, mating cycles and environment. We will propose material, temper and layer system and quote for your part.

- [Send an enquiry with drawing](https://www.atlas-contacte.de/en/request-a-quote/)
- [Surface finishes at ACA](https://www.atlas-contacte.de/en/services/surface-finishes/)

**Source:** [Contact Materials and Plating Compared | ACA Atlas Contacte](https://www.atlas-contacte.de/en/knowledge/materials-finishes/) · ACA Atlas Contacte GmbH, Wallbacher Straße 5, 79664 Wehr, Germany · Phone +49 7761 4420 · info@atlas-contacte.de · [Request a quote](https://www.atlas-contacte.de/en/request-a-quote/)